title: Overcoming Manufacturing Challenges for Next-Generation Copper Heat Exchanger Design
description: "One design feature is increasingly visible in the heat exchanger: smaller-diameter copper tubes, including internally enhanced or microgrooved designs."
image: https://blog.copper.org/hubfs/undefined-Nov-18-2026-02-07-50-0636-PM.png
---

[Skip to content](https://blog.copper.org/hvac/r/overcoming-manufacturing-challenges-for-next-generation-copper-heat-exchanger-design#main-content)

[![](https://blog.copper.org/hs-fs/hubfs/CDA_Logo_Copper_RGB.png?width=1118&height=256&name=CDA_Logo_Copper_RGB.png)](https://copper.org/)

Open main navigation

Close main navigation

- [Contact us](https://www.copper.org/about/contact.php)

[Contact us](https://www.copper.org/about/contact.php)

 Nov 18, 2026, 9:54:22 AM

# Overcoming Manufacturing Challenges for Next-Generation Copper Heat Exchanger Design

[Marcus Elmer](https://blog.copper.org/hvac/r/author/marcus-elmer)

Share: [facebook-f icon](http://www.facebook.com/share.php?u=https://blog.copper.org/hvac/r/overcoming-manufacturing-challenges-for-next-generation-copper-heat-exchanger-design) [linkedin-in icon](http://www.linkedin.com/shareArticle?mini=true&url=https://blog.copper.org/hvac/r/overcoming-manufacturing-challenges-for-next-generation-copper-heat-exchanger-design) [Twitter icon](https://twitter.com/intent/tweet?url=https://blog.copper.org/hvac/r/overcoming-manufacturing-challenges-for-next-generation-copper-heat-exchanger-design) [pinterest-p icon](http://pinterest.com/pin/create/link/?url=https://blog.copper.org/hvac/r/overcoming-manufacturing-challenges-for-next-generation-copper-heat-exchanger-design) [envelope icon](mailto:?body=https://blog.copper.org/hvac/r/overcoming-manufacturing-challenges-for-next-generation-copper-heat-exchanger-design)

**Overview**

- Low-GWP refrigerants and higher operating pressures are driving changes in HVAC/R heat exchanger design and material selection.
- Smaller-diameter copper tubing can reduce refrigerant charge and equipment size, but introduces manufacturing challenges related to tube handling, buckling, and expansion.
- Advanced expansion methods, including tubular hydro-expansion, help manufacturers produce smaller heat exchangers while minimizing tube shrinkage and preserving internal enhancements.
- High-strength copper-iron alloys and precision fabrication techniques support the production of manifolds and components for high-pressure CO2 refrigeration systems.
- Continued advances in tube geometry, automation, and manufacturing processes are expanding design possibilities for next-generation HVAC/R equipment.

HVAC/R equipment manufacturers are rethinking heat exchanger design as efficiency requirements, refrigerant transitions, and electrification reshape the industry. The move toward lower global warming potential (GWP) refrigerants presents opportunities to improve system performance, but it also introduces new engineering and manufacturing challenges.

Smaller-diameter copper tubing, advanced copper alloys, and evolving fabrication processes are helping manufacturers address these requirements. These technologies can reduce refrigerant charge, accommodate higher operating pressures, and support more compact heat exchanger designs.

During a [webinar hosted by the Copper Development Association (CDA)](https://blog.copper.org/hubfs/Manufacturing%20the%20Next%20Generation%20of%20HVACR%20Equipment%209.26.24.mp4?_hsenc=p2ANqtz-8d6nthpRugsfVlOT8yhmL-COzdphPGc89_kjMwt7aOkYdcoj1Ckj3cOIVqmpEghYYS4xLp), industry experts from [Burr Oak Tool](http://burroak.com/)and [T-DRILL](http://t-drill.com/)examined how copper materials and innovative manufacturing techniques are being used in next-generation HVAC/R equipment.

### **How Low-GWP Refrigerants Are Influencing Heat Exchanger Design**

The transition to [low-GWP refrigerants](https://blog.copper.org/hvac/r/navigating-the-future-of-refrigerants-epa-regulations-for-a3-flammable-refrigerants) is changing how manufacturers approach material selection, component design, and production.

Refrigerants such as R-32 and R-454B, along with natural refrigerants including R-290 (propane), R-600a (isobutane), and R-744 (carbon dioxide), introduce different considerations related to operating pressures, flammability, equipment efficiency, and system configuration.

Manufacturers must evaluate these requirements alongside production costs, material availability, and equipment performance.

##### **Copper offers several characteristics that make it suitable for evolving HVAC/R applications.**

- **Thermal conductivity:** Copper's high thermal conductivity supports heat transfer in heat exchangers and refrigeration components.
- **Formability and joining:** Copper tubing can be bent, expanded, brazed, and fabricated into complex configurations using established manufacturing processes.
- **Design flexibility:** Copper tubing is available in different diameters, wall thicknesses, and alloys to accommodate application-specific requirements.
- **Recyclability:** Copper can be recycled repeatedly without losing its inherent material properties, supporting circularity objectives.

[Smaller-diameter copper tubing](https://blog.copper.org/hvac/r/unlocking-the-advantages-of-lighter-weight-small-diameter-tubes) is particularly relevant as manufacturers seek to reduce refrigerant charge and equipment size while maintaining the necessary thermal performance.

### **Smaller-Diameter Copper Tubing and More Compact Heat Exchangers**

Round tube plate fin (RTPF) heat exchangers are widely used in HVAC/R equipment, including air conditioning evaporators, condensers, and mini-split systems.

These heat exchangers use tubing to circulate refrigerant through a series of fins, typically made from aluminum, that increase the surface area available for heat transfer. Manufacturers can modify tube diameter, fin geometry, and circuit configurations to meet specific performance requirements.

Historically, RTPF heat exchanger designs commonly used copper tubing with diameters of 5/8-inch, 1/2-inch, and 3/8-inch. More [recent designs](https://blog.copper.org/hvac/r/midea-split-air-conditioning-system-reduced-charge-with-4-mm-copper-tubes) have progressed toward 7 mm (millimeter), 5 mm, and even smaller diameters.

![ Evolution of copper tubing in HVAC/R heat exchangers](https://blog.copper.org/hs-fs/hubfs/undefined-Nov-18-2026-02-07-49-7845-PM.png?width=475&height=624&name=undefined-Nov-18-2026-02-07-49-7845-PM.png)

**Figure 1. Evolution of copper tubing in HVAC/R heat exchangers, illustrating the shift toward smaller tube diameters and denser tube configurations to increase heat transfer capacity while supporting more compact equipment designs. *Source: Burr Oak Tool, CDA webinar, “***[***Manufacturing the Next Generation of HVAC/R Equipment***](https://blog.copper.org/hubfs/Manufacturing%20the%20Next%20Generation%20of%20HVACR%20Equipment%209.26.24.mp4?_hsenc=p2ANqtz-8d6nthpRugsfVlOT8yhmL-COzdphPGc89_kjMwt7aOkYdcoj1Ckj3cOIVqmpEghYYS4xLp)***,” September 2024.***

Reducing the tube diameter can offer several advantages:

- **Lower refrigerant charge:** Smaller internal tube volumes can reduce the refrigerant required in a heat exchanger. This is particularly relevant as manufacturers evaluate systems using alternative refrigerants.
- **Compact equipment designs:** Smaller tubes allow manufacturers to develop denser tube arrangements and reduce the space required for certain heat exchanger configurations.
- **Improved design flexibility:** Manufacturers can adjust tube spacing, fin design, and refrigerant circuitry to optimize heat transfer for specific operating conditions.

These benefits depend on the complete heat exchanger design. Tube diameter must be evaluated alongside refrigerant-side pressure drop, airflow, thermal performance, and manufacturing feasibility.

### **Manufacturing Challenges With Small-Diameter Copper Tubing**

Although smaller copper tubes offer design advantages, their reduced dimensions introduce manufacturing challenges.

In a conventional RTPF production process, tubes and fins are assembled through lacing, followed by expansion, brazing, and forming. Each stage requires adjustments when manufacturing increasingly compact heat exchangers.

![Anatomy of a round tube plate fin (RTPF) heat exchanger](https://blog.copper.org/hs-fs/hubfs/undefined-Nov-18-2026-02-07-50-0636-PM.png?width=605&height=329&name=undefined-Nov-18-2026-02-07-50-0636-PM.png)

**Figure 2. Anatomy of a round tube plate fin (RTPF) heat exchanger, illustrating the key components, including copper hairpin tubes, return bends, fins, and end sheets, that work together to circulate refrigerant, facilitate heat transfer, and provide structural support. Source: Burr Oak Tool, CDA webinar, “**[**Manufacturing the Next Generation of HVAC/R Equipment**](https://blog.copper.org/hubfs/Manufacturing%20the%20Next%20Generation%20of%20HVACR%20Equipment%209.26.24.mp4?_hsenc=p2ANqtz-8d6nthpRugsfVlOT8yhmL-COzdphPGc89_kjMwt7aOkYdcoj1Ckj3cOIVqmpEghYYS4xLp)**,” September 2024.**

##### **Fin Production and Tube Handling**

Smaller tube diameters require smaller fin openings and more precise alignment during assembly.

In fin production, smaller stacking rods have reduced strength and can be more susceptible to deflection. During the [webinar](https://blog.copper.org/hubfs/Manufacturing%20the%20Next%20Generation%20of%20HVACR%20Equipment%209.26.24.mp4?_hsenc=p2ANqtz-8d6nthpRugsfVlOT8yhmL-COzdphPGc89_kjMwt7aOkYdcoj1Ckj3cOIVqmpEghYYS4xLp), Burr Oak Tool highlighted several approaches to address these challenges, including improved stacker rod materials, optimized rod-tip geometry, and remote feed-and-cutoff systems that reduce vibration during stacking.

Hairpin production also becomes more complex. Longer, thinner tubes have lower column strength, making them more susceptible to bending or buckling during handling.

Stretch straightening, additional tube supports, and automated handling systems can help manufacturers maintain dimensional accuracy and manage higher production volumes.

##### **Tube Expansion**

Tube expansion is another critical manufacturing operation. During mechanical expansion, a tool is passed through the tubing to expand its diameter and establish contact with the surrounding fins. This connection supports effective heat transfer between the tube and fin surfaces.

As tube diameter decreases, the tubing generally becomes more resistant to circumferential expansion while becoming more susceptible to axial buckling under compressive loads.

Manufacturers must also control tube deformation to avoid damaging internal surface enhancements designed to improve heat transfer.

These limitations have encouraged the development of alternative expansion technologies.

### **Advancing Copper Tube Expansion Technologies**

Burr Oak Tool examined several tube-expansion approaches to address the challenges associated with small-diameter tubing.

| **EXPANSION METHOD** | **MANUFACTURING CONSIDERATIONS** |
| --- | --- |
| Conventional compression expansion | Can cause coil buckling and approximately 3% to 5% shrinkage, with practical limitations for tubes smaller than 5 mm. |
| Tension expansion | Reduces the risk of buckling and limits shrinkage to approximately 2%-3%, but requires more expensive tooling. |
| Limited-shrink tension expansion | Can reduce shrinkage to approximately 0-1%, although tooling costs and diameter limitations remain. |
| Pressure expansion | Uses internal pressure to expand tubing, enabling zero-shrink expansion and accommodating tubes smaller than 5 mm. |

**Source: Burr Oak Tool presentation during CDA's** [**Manufacturing the Next Generation of HVAC/R Equipment webinar**](https://blog.copper.org/hubfs/Manufacturing%20the%20Next%20Generation%20of%20HVACR%20Equipment%209.26.24.mp4?_hsenc=p2ANqtz-8d6nthpRugsfVlOT8yhmL-COzdphPGc89_kjMwt7aOkYdcoj1Ckj3cOIVqmpEghYYS4xLp)**. Shrinkage figures reflect the methods presented and should not be interpreted as universal production results.**

Pressure expansion, also called tubular hydro-expansion, is particularly relevant to smaller-diameter heat exchangers. Unlike conventional mechanical expansion, which relies on an internal tool to deform the tube, pressure expansion applies force through internal pressure.

This approach can eliminate axial shrinkage and help preserve internal tube enhancements that might otherwise be damaged during mechanical expansion. Advances in these manufacturing processes are enabling the use of smaller tubing and more complex internal geometries in future heat exchanger designs.

### **Copper Alloys for High-Pressure CO2 Refrigeration Systems**

The growing use of carbon dioxide refrigerant, designated R-744, introduces additional material requirements.

CO2 has a GWP of 1 and an ozone depletion potential of zero. However, CO2 refrigeration systems, particularly those operating in transcritical configurations, can experience substantially higher pressures than many conventional refrigeration systems.

These conditions require manufacturers to consider the strength and pressure ratings of tubing, fittings, manifolds, and connections.

**Copper-iron alloys** offer one potential solution.

For example, copper-iron alloy UNS C19400 provides enhanced mechanical strength compared with conventional copper tubing, making it relevant to high-pressure refrigeration applications.

Material selection must account for operating temperatures, design pressures, wall thickness, joining methods, and applicable equipment standards.

The availability of specialized copper alloys and fabrication technologies enables manufacturers to evaluate copper-based solutions for demanding refrigeration applications without relying solely on thicker tube walls.

### **Advanced Tube Fabrication for Refrigeration Manifolds**

Manufacturing improvements extend beyond heat exchanger coils. Refrigeration systems also require manifolds and headers to distribute refrigerant through multiple circuits. Producing these components involves creating precise openings, forming branch connections, and ensuring reliable joints.

During the [webinar](https://blog.copper.org/hubfs/Manufacturing%20the%20Next%20Generation%20of%20HVACR%20Equipment%209.26.24.mp4?_hsenc=p2ANqtz-8d6nthpRugsfVlOT8yhmL-COzdphPGc89_kjMwt7aOkYdcoj1Ckj3cOIVqmpEghYYS4xLp), T-DRILL highlighted several tube fabrication techniques used in the production of copper and copper-alloy manifolds, including punching and collaring, friction drilling, tube-end spinning, and precision cutting.

Collaring processes form branch connections directly from the parent tube wall. This can simplify certain manifold designs and reduce the need for separate branch fittings.

Precision cutting and forming are also important in maintaining the consistency required for subsequent joining operations.

For higher-pressure refrigeration systems, manufacturers must validate finished components and joints against the intended operating conditions. Fabrication methods, material strength, and connection design all influence the final assembly’s pressure integrity.

**![Examples of advanced copper tube fabrication techniques](https://blog.copper.org/hs-fs/hubfs/undefined-Nov-18-2026-02-07-50-5725-PM.png?width=510&height=413&name=undefined-Nov-18-2026-02-07-50-5725-PM.png)**

**Figure 3. Examples of advanced copper tube fabrication techniques, including precision cutting, punching and collaring, used to produce manifolds and branch connections for HVAC/R applications. Source: T-DRILL, CDA webinar, “**[**Manufacturing the Next Generation of HVAC/R Equipment**](https://blog.copper.org/hubfs/Manufacturing%20the%20Next%20Generation%20of%20HVACR%20Equipment%209.26.24.mp4?_hsenc=p2ANqtz-8d6nthpRugsfVlOT8yhmL-COzdphPGc89_kjMwt7aOkYdcoj1Ckj3cOIVqmpEghYYS4xLp)**,” September 2024.**

### **What’s Next for Copper Heat Exchanger Manufacturing?**

As HVAC/R manufacturers continue developing equipment for alternative refrigerants, heat exchanger production technologies will need to accommodate increasingly demanding geometries.

The Burr Oak Tool presentation identified several areas of continued development, including tubing smaller than 4 mm, new internal tube enhancements, and non-round tube configurations. These developments could expand design possibilities, but their commercial viability will depend on manufacturing consistency, tooling capabilities, and demonstrated performance.

Copper’s combination of thermal conductivity, formability, and available alloy options provides manufacturers with flexibility as they evaluate these emerging technologies.

The opportunity is to consider material selection and manufacturing processes together during product development. A smaller tube diameter or higher-strength alloy may enable a new design, but the resulting heat exchanger must still meet thermal, mechanical, safety, and production requirements.

> **For North American HVAC/R manufacturers evaluating enhanced small-diameter copper tubes, the Copper Development Association offers research, development, and** [**technical support**](https://blog.copper.org/hvac/r/5-reasons-to-partner-with-the-copper-development-association-for-research-and-development-to-develop-the-next-generation-of-heat-exchangers) **through CDA and its network of industry experts. Manufacturers can work with the network on projects involving heat exchanger design, simulation, testing, and evaluation, helping teams assess concepts and optimize designs before commercialization.**
> 
> **[Learn how to partner with CDA](https://info.copper.org/how-to-partner-with-cda?utm_source=chatgpt.com)**

## **Frequently Asked Questions**

What technological advancements are influencing HVAC systems today?

Advancements in heat exchanger design, low global warming potential (GWP) refrigerants and manufacturing processes are shaping next-generation HVAC/R systems. Smaller-diameter copper tubing enables more compact heat exchangers with reduced refrigerant charge, while advanced copper alloys support higher-pressure applications such as CO2 refrigeration. Innovations in tube expansion, automation, and precision fabrication are also helping manufacturers improve production efficiency and accommodate increasingly complex equipment designs.

Why is copper used in HVAC/R heat exchangers?

Copper is widely used because of its high thermal conductivity, formability, and established joining methods. It can be fabricated into complex tubing configurations and is available in various diameters, wall thicknesses, and alloys to accommodate a range of operating conditions.

How does smaller-diameter copper tubing reduce refrigerant charge?

Smaller-diameter tubing has less internal volume per unit length than larger tubing. When incorporated into an appropriately designed heat exchanger, it can reduce the required refrigerant volume. Actual refrigerant savings depend on the system’s overall design and configuration.

Can copper tubing be used with low-GWP refrigerants?

Yes. Copper and selected copper alloys can be used with various low-GWP refrigerants, provided the tubing, joints and other system components meet the refrigerant’s operating pressure, temperature and compatibility requirements.

What are the advantages of copper-iron alloys in CO2 refrigeration?

Copper-iron alloys offer greater mechanical strength than conventional copper tubing. This makes appropriately specified alloys suitable for consideration in high-pressure CO2 refrigeration applications, including certain manifolds and heat exchanger components.

 

### Marcus Elmer

***Vice President and Director, Tube & Fittings Council***

*Marcus Elmer is a seasoned professional with over 15 years of experience in the plumbing and mechanical industries. He leverages his expertise to identify and influence market trends for copper tube and fittings products, driving strategic programs encompassing technical research, codes and standards, advocacy, and education. With a unique perspective gained from his time as a project manager with commercial plumbing, mechanical, and refrigeration contractors, Elmer has a deep understanding of the industry.*

 

[small diameter copper tube heat exchangers](https://blog.copper.org/hvac/r/tag/small-diameter-copper-tube-heat-exchangers), [small diameter copper tube](https://blog.copper.org/hvac/r/tag/small-diameter-copper-tube), [Heat Exchangers](https://blog.copper.org/hvac/r/tag/heat-exchangers), [Small-Diameter Copper Tube for Heat Exchangers](https://blog.copper.org/hvac/r/tag/small-diameter-copper-tube-for-heat-exchangers), [copper tubes](https://blog.copper.org/hvac/r/tag/copper-tubes), [5mm copper tube](https://blog.copper.org/hvac/r/tag/5mm-copper-tube), [sustainable hvac/r](https://blog.copper.org/hvac/r/tag/sustainable-hvac-r), [energy efficiency](https://blog.copper.org/hvac/r/tag/energy-efficiency), [new refrigerants](https://blog.copper.org/hvac/r/tag/new-refrigerants), [Low GWP Refrigerants](https://blog.copper.org/hvac/r/tag/low-gwp-refrigerants), [copper heat exchanger manufacturing](https://blog.copper.org/hvac/r/tag/copper-heat-exchanger-manufacturing)

## Related posts

[![Enhanced Small-Diameter Copper Tubes in Heat Exchangers](https://blog.copper.org/hs-fs/hubfs/image2.png?height=200&name=image2.png)](https://blog.copper.org/hvac/r/the-global-shift-to-enhanced-small-diameter-copper-tubes)

## [The Global Shift to Enhanced Small-Diameter Copper Tubes in Heat Exchangers](https://blog.copper.org/hvac/r/the-global-shift-to-enhanced-small-diameter-copper-tubes)

[Marcus Elmer](https://blog.copper.org/hvac/r/author/marcus-elmer) 

 Aug 17, 2026, 11:15:45 AM

Overview Global cooling demand is rising rapidly, pushing HVAC/R manufacturers to improve...

[Read more](https://blog.copper.org/hvac/r/the-global-shift-to-enhanced-small-diameter-copper-tubes)

[![](https://blog.copper.org/hs-fs/hubfs/Condenser_5mm_1.png?height=200&name=Condenser_5mm_1.png)](https://blog.copper.org/hvac/r/understanding-inner-grooved-small-diameter-copper-tube-heat-exchangers-design-benefits-and-applications)

## [Understanding Inner-Grooved, Small-Diameter Copper Tube Heat Exchangers: Design, Benefits, and Applications](https://blog.copper.org/hvac/r/understanding-inner-grooved-small-diameter-copper-tube-heat-exchangers-design-benefits-and-applications)

[Marcus Elmer](https://blog.copper.org/hvac/r/author/marcus-elmer) 

 Jun 22, 2026, 1:37:47 PM

By Marcus Elmer, Vice President and Director, Tube & Fittings Council for the Copper Development...

[Read more](https://blog.copper.org/hvac/r/understanding-inner-grooved-small-diameter-copper-tube-heat-exchangers-design-benefits-and-applications)

[![](https://blog.copper.org/hs-fs/hubfs/R454B%20Unit%20from%20AHR%20Expo%202025%20HTT%20report.jpeg?height=200&name=R454B%20Unit%20from%20AHR%20Expo%202025%20HTT%20report.jpeg)](https://blog.copper.org/hvac/r/inside-ahr-2025-how-small-diameter-copper-tubes-are-shaping-the-future)

## [Inside AHR 2025: How Small-Diameter Copper Tubes are Shaping the Future of System Design](https://blog.copper.org/hvac/r/inside-ahr-2025-how-small-diameter-copper-tubes-are-shaping-the-future)

[Marcus Elmer](https://blog.copper.org/hvac/r/author/marcus-elmer) 

 Jun 17, 2025, 10:44:10 AM

Each year, the AHR Expo acts as a window into the future of the HVACR industry. In 2025, that...

[Read more](https://blog.copper.org/hvac/r/inside-ahr-2025-how-small-diameter-copper-tubes-are-shaping-the-future)

[facebook-f icon](https://www.facebook.com/CopperDevelopment) [linkedin-in icon](https://www.linkedin.com/company/2658439/) [Twitter icon](https://twitter.com/thinkcopperUS)

---

[![CDA\_Logo\_Copper\_RGB](https://blog.copper.org/hs-fs/hubfs/CDA_Logo_Copper_RGB.png?width=250&height=57&name=CDA_Logo_Copper_RGB.png "CDA_Logo_Copper_RGB")](https://www.copper.org/)

Copyright © 2026, Copper Development Association

```json
{
  "@context" : "https://schema.org",
  "@type" : "BlogPosting",
  "author" : {
    "@type" : "Person",
    "name" : "Marcus Elmer",
    "url" : "https://blog.copper.org/hvac/r/author/marcus-elmer"
  },
  "dateModified" : "2026-11-18T14:54:22.304Z",
  "datePublished" : "2026-11-18T14:54:22.000Z",
  "headline" : "Overcoming Manufacturing Challenges for Next-Generation Copper Heat Exchanger Design",
  "image" : [ "https://blog.copper.org/hubfs/undefined-Nov-18-2026-02-07-50-0636-PM.png" ],
  "mainEntityOfPage" : {
    "@id" : "https://blog.copper.org/hvac/r/overcoming-manufacturing-challenges-for-next-generation-copper-heat-exchanger-design",
    "@type" : "WebPage"
  },
  "publisher" : {
    "@type" : "Organization",
    "logo" : {
      "@type" : "ImageObject",
      "url" : "https://blog.copper.org/hubfs/CDA_Logo_Copper_RGB.png"
    },
    "name" : "Copper Development Association"
  }
}
```